Stellite 6 weld overlay is the process of depositing a layer of Stellite 6, a cobalt-chromium alloy strengthened by a network of chromium carbides, onto a carbon or low-alloy steel base component, instead of manufacturing the entire part from solid Stellite 6. 

For valve trim, seating surfaces, and other components exposed to sliding wear, galling, or elevated-temperature service, this delivers the alloy’s characteristic hardness and wear resistance exactly where the component needs it, at a fraction of the material cost and lead time of a solid cobalt-alloy part.

If your project is still deciding between a solid Stellite 6 component and a TIG- or GMAW-applied overlay, it's worth reviewing the wear mechanism and operating envelope with an engineering team before locking in the material specification.

Why Stellite 6 overlay instead of a solid component

A component machined entirely from solid Stellite 6 is rarely the most efficient way to solve a wear problem: the alloy is a cobalt-based material that costs a multiple of carbon or low-alloy steel, and the hardness is only needed on the surface that actually contacts the mating part or the process media. 

Stellite 6 is specified when a working surface must resist abrasive and adhesive wear, galling and, depending on service, elevated temperature, typically on valve seats, valve trim and other sliding or high-wear surfaces.

Weld overlay, also referred to as cladding, solves this by depositing a layer of Stellite 6, typically a few millimetres thick, onto a structural carbon or low-alloy steel base. The base material carries the mechanical load and machinability; the Stellite 6 layer carries the wear resistance. Because Stellite 6 gets its performance from a carbide network rather than from solid-solution strengthening, where it is not the right choice matters just as much as where it is. Let’s talk about it.

Welding processes for Stellite 6 overlay: TIG (GTAW), Tiger and GMAW compared

Deciding between TIG and GMAW for a specific valve component or fitting is easiest with the drawing and the service conditions in hand. MEGA’s cladding team can confirm which process fits your geometry and dilution requirement.

Typical Stellite 6 weld overlay procedure, step by step

Stellite 6 weld overlay

Typical Stellite 6 weld overlay procedure, step by step

A procedure that looks fine on paper but skips a single verification step is precisely where a Stellite 6 overlay project runs into trouble at the qualification stage. A qualified procedure follows a defined sequence.

Preparation · 1–3Welding · 4Verification · 5–6Qualification · 7
1

Preparation

Base material selection and preparation

The substrate is cleaned and prepared to remove oxides and contaminants before welding.

C-Mn steelLow-alloy steelHigh-alloy steelMartensitic / ferritic stainless
2

Preparation

Filler metal and process selection

A Stellite 6 (cobalt-chromium-tungsten-carbon) filler wire or rod, deposited according to the component’s geometry and size.

GTAWHot-wire GTAW / TigerGMAW
3

Preparation

Thermal control

Stellite 6 deposits are generally more crack-sensitive than nickel-based overlays, so preheat and a controlled interpass temperature are commonly required on hardenable steel substrates.

Exact values follow the qualified WPS for the specific base/filler combination: they vary by supplier, base material and governing code.

4

Welding

Deposition

Single- or multi-layer deposition, with the cladding orientation chosen by part shape.

Horizontal: 2 layers in one pass · pipes & long productsVertical: rotating head · asymmetrical parts
5

Verification

Dilution and hardness verification

Chemical analysis and hardness testing confirm the deposited layer’s carbide content and hardness meet the qualified procedure, not just the nominal filler chemistry.

6

Verification

Non-destructive testing

Verifies bond integrity and surface soundness.

Visual inspectionPTUTMT
7

Qualification

Documentation

The WPS is qualified with a PQR per ASME Section IX (or the equivalent code the project specifies), with full material traceability delivered alongside the finished part.

Confirming a Stellite 6 overlay procedure before it is qualified is far cheaper than requalifying it after a failed PQR. Reviewing the parameters against your project’s design code before welding starts is worth the time.

Talk to our cladding team

A procedure that looks fine on paper but skips a single verification step is precisely where a Stellite 6 overlay project runs into trouble at the qualification stage. A qualified procedure follows a defined sequence:

  • Base material selection and preparation: the substrate (C-Mn steel, low-alloy steel, high-alloy steel, or martensitic/ferritic stainless steel) is cleaned and prepared to remove oxides and contaminants before welding.
  • Filler metal and process selection: a Stellite 6 (cobalt-chromium-tungsten-carbon) filler wire or rod, deposited via GTAW, hot-wire GTAW/Tiger, or GMAW depending on the component’s geometry and size.
  • Thermal control: Stellite 6 deposits are generally more crack-sensitive than nickel-based overlays, so preheat and a controlled interpass temperature are commonly required on hardenable steel substrates; the exact values follow the qualified WPS for the specific base/filler combination, since they vary by supplier, base material and governing code.
  • Deposition: single- or multi-layer, using horizontal cladding (two layers in one pass of the welding head) for pipes and long products, or vertical cladding (rotating head) for asymmetrical parts.
  • Dilution and hardness verification: chemical analysis and hardness testing confirm the deposited layer’s carbide content and hardness meet the qualified procedure, not just the nominal filler chemistry.
  • Non-destructive testing: visual inspection, penetrant testing (PT), ultrasonic testing (UT) and magnetic particle testing (MT) verify bond integrity and surface soundness.
  • Documentation: the WPS is qualified with a PQR per ASME Section IX (or the equivalent code the project specifies), with full material traceability delivered alongside the finished part.

Confirming a Stellite 6 overlay procedure before it is qualified is far cheaper than requalifying it after a failed PQR. Reviewing the parameters against your project’s design code before welding starts is worth the time.

Dilution, cracking and hardness: where Stellite 6 overlay does and doesn’t make sense

A Stellite 6 overlay is only as reliable as its most inconsistent pass, and the variable that most often gets overlooked in general weld-overlay content is that dilution affects Stellite 6 differently than it affects a corrosion-resistant alloy like Inconel 625. Three points are worth specifying:

  • Dilution and hardness: because Stellite 6’s wear resistance comes from its carbide network rather than from a solid-solution matrix, excessive dilution from the base metal does not just shift the chemistry: it directly lowers the deposit’s hardness and wear performance, which is why hardness testing, not only chemical analysis, is a standard verification step for Stellite 6 overlays.

  • Cracking risk: Stellite 6 is generally more crack-sensitive than nickel-based overlay alloys, particularly on hardenable or higher-carbon steel substrates; preheat, controlled interpass temperature, and, on some specifications, post-weld heat treatment reduce this risk and should be defined in the qualified welding procedure rather than assumed.

  • Where Stellite 6 overlay is not the right choice: on components exposed primarily to uniform corrosive attack rather than mechanical wear, sliding contact, or galling, a nickel-based overlay such as Inconel 625 is typically the better-suited material. Stellite 6 should be specified for its wear and galling resistance, not treated as a general-purpose corrosion solution, a distinction almost no published Stellite 6 content spells out, and one worth confirming against your component’s actual failure mode before the material is locked in.

If your specification is still undecided between a wear-resistant and a corrosion-resistant overlay, walking through the component’s dominant failure mode with MEGA’s engineering team before the procedure is qualified avoids specifying the wrong alloy for the job.

 

Beyond valves: applying Stellite 6 overlay to elbows, tees, reducers, and caps

Any fitting geometry that sees erosive wear or particulate-laden flow is a legitimate cladding candidate, and MEGA’s cladding division applies Stellite 6 overlay across the fitting types it forges and machines in-house:

  • Elbows (45° and 90°): used to change the direction of flow; long-radius elbows are preferred to reduce friction and erosion, and overlaying the bore protects exactly the surface where a directional change concentrates turbulence and particulate impact.

  • Tees (equal and reducing): used to create branch lines; a branch connection is a natural point of flow disturbance, and overlaying the run and branch bore extends service life at the geometry most exposed to erosive wear.

  • Reducers (concentric and eccentric): used to change pipe diameter; eccentric reducers are critical in horizontal suction lines to prevent air pockets, and the same wear-resistant layer that protects a straight run can be applied to the reducer that connects it.

  • Caps and plugs: used to seal the end of a pipe or a branch; in some layouts a cap or plug still sees erosive flow at the terminus, making the material at this point as relevant as the rest of the line.

Standards to check for a Stellite 6 weld overlay supplier

Because a Stellite 6 overlay is difficult to fully re-inspect once a component is installed, the supplier’s qualification and quality framework matters as much as the alloy itself:

  • Filler metal classification: cobalt-base (Stellite-type) surfacing filler metals are commonly classified under AWS A5.21 (bare electrodes and rods for surfacing); confirm the exact designation with the filler and process supplier.

  • Welding procedure qualification: WPS and PQR qualified per ASME Section IX, or the equivalent qualification code the project specifies.

  • The governing design code for the component: for MEGA’s fitting range, this includes ASME B31.1, B31.3, B31.4 and B31.8, ASME BPV Code Sections I, III and VIII (Divisions 1 and 2), PED, RCC-M, EN 13480 and EN 10253, depending on the project and jurisdiction.

  • Hardness and wear verification: a hardness survey across the overlay, the heat-affected zone and the base metal is a standard check for wear-resistant overlays; confirm which acceptance criteria and, where relevant, abrasion or galling test methods the supplier tests against.

 

Talk to MEGA about your Stellite 6 weld overlay requirement

Whether a component needs a solid Stellite 6 body, a Stellite 6 weld overlay, or a different overlay alloy entirely, that decision is easiest to get right before the procedure is qualified and the material specification is locked in. MEGA’s cladding division and engineering team can review the base material, the geometry, and the certification package your project requires, on valve-related components, but also on the elbows, tees, reducers and caps a typical Stellite overlay conversation usually skips.

Contact MEGA’s technical sales team to discuss your Stellite 6 weld overlay requirement.

Frequently Asked Questions

Is Stellite 6 harder than Inconel 625?

Generally, yes, for wear-resistance purposes. Stellite 6’s hardness comes from a network of chromium carbides in a cobalt matrix, which typically gives it higher as-deposited hardness and better resistance to abrasive and adhesive wear than a solid-solution-strengthened nickel alloy such as Inconel 625. Inconel 625, in turn, is chosen for uniform corrosion resistance rather than wear resistance. The two alloys solve different problems, and the right choice depends on which failure mode the component actually faces.

What is weld overlay?

Weld overlay is the process of depositing a layer of a different alloy, here Stellite 6, onto a structural base material using an arc-welding process, so the finished component gets the deposited alloy’s surface properties (in this case, wear and galling resistance) without being manufactured entirely from that alloy. It is also referred to as cladding.

Is Stellite expensive?

Stellite 6 is a cobalt-based alloy and costs significantly more than carbon or low-alloy steel per kilogram. Applying it as a thin overlay, typically a few millimetres thick, rather than manufacturing an entire component from solid Stellite 6, is what keeps the total component cost manageable, the same logic that applies to other overlay alloys such as Inconel 625.

What is Stellite 6 used for?

Stellite 6 is used on components whose working surface must resist sliding wear, galling and, depending on service, elevated temperature, most commonly valve seats and valve trim, as well as other high-wear surfaces in oil & gas, petrochemical, and power generation equipment. It is specified for wear and galling resistance rather than as a general corrosion solution.

Can Stellite 6 overlay be applied to fittings and forgings, not just valve components?

Yes. MEGA’s cladding division applies Stellite 6 overlay to forgings, fittings and flanges as well as pipes up to 12 metres in length, using the same horizontal or vertical Tiger cladding equipment, or GMAW, matched to the component’s geometry.